ï¼1ï¼ å²å»å¼ºåº¦ç¨äºè¯ä»·ææçæå²å»è½åæå¤æææçèæ§åé§æ§ç¨åº¦ï¼å æ¤å²å»å¼ºåº¦ä¹ç§°å²å»é§æ§ã
ï¼2ï¼ å²å»å¼ºåº¦æ¯è¯æ ·å¨å²å»ç ´åè¿ç¨ä¸æå¸æ¶çè½éä¸åå§æ¨ªæªé¢ç§¯ä¹æ¯ã
ï¼3ï¼å²å»å¼ºåº¦çæµéæ å主è¦æISOå½é
æ åï¼GBåç
§ISOï¼åç¾å½ææASTMæ åã
(4) æ常è§çå²å»å¼ºåº¦æµè¯æ¯å¡æå¶åçå²å»å¼ºåº¦ã
æ ¹æ®è¯éªè®¾å¤ä¸åå¯å为ç®æ¯æ¢å²å»å¼ºåº¦ãæ¬èæ¢å²å»å¼ºåº¦.
GB/T 1043.1-2008 å¡æ.ç®æ¯æ¢å²å»æ§è½çæµå®.第1é¨å:é仪å¨åå²å»è¯éª [1] ASTM D6110-2010 Standard Test Method for Determining the Charpy Impact Resistance of Notched Specimens of Plastics[2] è§å®äºå¡æå¨è§å®æ¡ä»¶ä¸æµå®ç®æ¯æ¢å²å»å¼ºåº¦çæ¹æ³ã
GB/T 1843-2008 å¡æãæ¬èæ¢å²å»å¼ºåº¦çæµå®[3] [3] å ASTM D256-2010 Standard Test Methods for Determining the Izod Pendulum Impact Resistance of Plastics[4] è§å®äºå¡æå¨è§å®æ¡ä»¶ä¸æµå®ç®æ¯æ¢å²å»å¼ºåº¦çæ¹æ³ã
å
·ä½åºåå¦ä¸ï¼
GB: æ¯è¯ä»¶å¨ä¸æ¬¡å²å»å®éªæ¶ï¼åä½æ¨ªæªé¢ç§¯ï¼m2ï¼ä¸ææ¶èçå²å»åï¼Jï¼ï¼å
¶åä½ä¸ºMJ/m2ã
ASTM:å®åæ äºæææµæè£çº¹æ©å±åæèæçè½å,åä½å®½åº¦ææ¶èçåï¼åä½ä¸ºJ/mã
设å¤åºåï¼
æ¬èæ¢å²å»æ¹åä¸é´ææéï¼ç®æ¯æ¢å²å»æ¹ååç´é¢æå¹åï¼æ£é¢å½¢ç¶ä¸ºä¸å¹å½¢æé¤ã
缺å£åºåï¼
缺å£ä¸è¬å为åç§ï¼æVåå£åUåå£ä¸¤ç§ï¼æ¯ç§æ ¹æ®ç®çå弧åå¾åå为两ç§ã
æ ·æ¡åºåï¼
GBï¼ä¸è¬ä¸º 80*10mm æ ·æ¡ ä»¥å63.5*10mm æ ·æ¡ ç¼ºå£ä¸º2mmï¼ä¹æ63.8*12.7mmæ ·æ¡
ATSM:ä¸è¬ä¸º63.5*12.7mm 缺å£å©ä½å®½åº¦ä¸º 10.16mm ï¼å½å
æç¨80*10æ ·æ¡ï¼
æµè¯å
¬å¼ï¼
GB: a=W / (h*d) åä½KJ/m2 ATSM: a= W /d åä½ï¼J/m
a:å²å»å¼ºåº¦
W :å²å»æ失è½é
hï¼ç¼ºå£å©ä½å®½åº¦
dï¼æ ·æ¡å度
å æ¤ï¼GBä¸ASTMä¹é´ä¸å¯ä»¥çåæµéï¼ä½ä»æµéå
¬å¼å¯æ»ç»ç»éªå
¬å¼ï¼GBæ°å¼*10.16æ8ï¼éè¯¯æ ·æ¡ï¼=ASTMæ°å¼ï¼ä¹å¯ä»¥ç±å®é
æµéæ¥æ»ç»æ¯å¼ã
(5) é¤å»å¡æå²å»å¼ºåº¦ä¹å¤ï¼å¸¸ç¨çå²å»å¼ºåº¦è¿æï¼
GB/T 229-2007éå±ææ å¤æ¯æé¤å²å»è¯éªæ¹æ³
GB/T 13465.4-2014ä¸éæ§ç³å¢¨ææè¯éªæ¹æ³ 第4é¨å:å²å»å¼ºåº¦
SJ/T 11041-1996çµåç»çæå²å»å¼ºåº¦æµè¯æ¹æ³
HG/T 3845-2008硬质橡è¶.å²å»å¼ºåº¦çæµå®
JB/T 7609-2006çç³å¢¨æææå²å»å¼ºåº¦è¯éªæ¹æ³